SUS316 vs SUS304: Composition, Performance and Selection Guide
Aug 12, 2025
एक संदेश छोड़ें
SUS304 and SUS316: The Two Workhorses of Austenitic Stainless Steel
SUS304 is the JIS designation of 18-8 austenitic stainless steel, roughly 18% chromium and 8% nickel, and it is the most widely used stainless steel for food, chemical and household applications. SUS316 is the molybdenum-bearing JIS grade with 16-18% chromium, 10-14% nickel and 2-3% molybdenum, specified where chlorides and acids demand higher corrosion resistance, such as marine, chemical and medical equipment. Both are austenitic, non-magnetic in the annealed condition, and easy to form and weld.
Chemical Composition (JIS G4303)
Composition ranges per JIS G4303 for SUS304 and SUS316, in weight percent:
| SUS304 | SUS316 | |
|---|---|---|
| 18.00-20.00 | 16.00-18.00 | |
| 8.00-10.50 | 10.00-14.00 | |
| 2.00-3.00 | ||
| 0.08 max | 0.08 max | |
| 1.00 max | 1.00 max | |
| 2.00 max | 2.00 max | |
| 0.045 max | 0.045 max | |
| 0.030 max | 0.030 max |
| SUS304 | SUS316 | |
|---|---|---|
| 520 MPa min | 520 MPa min | |
| Yield Strength (0.2% offset) | 205 MPa min | 205 MPa min |
| 40% min | 40% min | |
| Density (g/cm3) | 7.93 | 7.98 |
| About 870 degrees C | About 870-925 degrees C |
The molybdenum in SUS316 is the single most important difference. Molybdenum strengthens the passive film and suppresses the initiation of pitting and crevice corrosion in chloride media, so SUS316 is the standard choice for seawater contact, coastal installations, road-salt exposure and many chemical process streams. The pitting resistance equivalent number (PREN=Cr + 3.3 Mo + 16 N) of SUS316 is about 25, versus about 19 for SUS304. Neither grade should be used in hot, concentrated acids; nickel-base or high-molybdenum alloys are required there.
Both grades are austenitic and essentially non-magnetic after annealing. Cold working, machining or welding can transform part of the structure to martensite, producing weak magnetism, with SUS304 slightly more susceptible than SUS316. Both grades weld readily by TIG or MIG without post-weld heat treatment, provided matching or low-carbon filler such as ER316L is used for SUS316 to preserve weld-zone corrosion resistance. For continuous service, the practical oxidation limit of both grades is about 870-925 degrees C; SUS316 has modestly better high-temperature strength, and both retain toughness at low temperatures down to about -200 degrees C where impact testing demonstrates compliance.
Choose SUS304 for general, indoor or mild service: kitchen equipment, food processing, decorative panels, plumbing fixtures, where economy matters.
Choose SUS316 for saltwater, coastal, high-chloride or chemical service: offshore platforms, desalination plants, chemical storage tanks, marine hardware, heat exchangers with chloride-bearing cooling water.
SUS316 typically costs 20-40% more than SUS304, so it is specified only when the environment justifies the premium.
What is the main difference between SUS316 and SUS304? SUS316 contains 2-3% molybdenum, which gives markedly better resistance to pitting and crevice corrosion in chloride environments; SUS304 contains no molybdenum.
Is SUS316 better than SUS304? In corrosion resistance, yes, especially in chloride and acid media. In cost, no: SUS316 typically costs 20-40% more. The right grade depends on the environment.
Are SUS304 and SUS316 magnetic? Both are essentially non-magnetic in the annealed condition. Cold working or welding can induce weak magnetism, more easily in SUS304 than in SUS316.
Can SUS316 be welded without post-weld heat treatment? Yes. SUS316 and SUS304 are welded by TIG or MIG without PWHT; using low-carbon filler such as ER316L maintains corrosion resistance in the weld zone.
What is the temperature limit for SUS316 and SUS304? Continuous service is typically limited to about 870-925 degrees C by oxidation; above that, scaling accelerates. For pressure design above about 550 degrees C, allowable stresses must be checked against code tables.
SUS316. SUS304 will pit and crevice-corrode in seawater; SUS316 is the minimum recommended austenitic grade for marine service, and for warm or stagnant seawater, duplex or super-duplex grades are safer.